A four-pigment study finds most natural colorants survive twin-screw extrusion and injection molding with limited rheology and mechanical penalties, while lightfastness and spirulina's thermal sensitivity remain the main constraints.

Mirela ConstantinNovember 2, 20265 min read9 views

Four colored polymer strands leave a laboratory extruder die and enter a cooling bath, next to dishes of plant-based pigment powder and molded plastic test bars.

A study has assessed whether four commercial natural pigments can be turned into color masterbatches and processed in biodegradable polyesters on conventional equipment. Blue spirulina, yellow curcumin, red beetroot and green chlorophyllin were compounded with polylactic acid (PLA) and polybutylene succinate (PBS) by twin-screw extrusion, then let down into the matching polymer at 2, 4 and 6 wt% and injection molded into test specimens. The masterbatch formulations also contained titanium dioxide, calcium carbonate and stearic acid, added to support UV protection, pigment dispersion and processing.

Heat is the central obstacle. The organic pigments begin to degrade at lower temperatures than the polymers that carry them. Thermogravimetric analysis put the degradation onset at about 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, while PLA and PBS showed considerably higher degradation temperatures. The researchers therefore selected extrusion profiles that melted each polymer while limiting the pigments' thermal exposure.

Processing reached 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h. Most pigment–polymer combinations fitted inside this window, but spirulina did not: during PLA processing it lost its characteristic blue, so a blue PLA masterbatch could not be produced. In PBS, whose lower processing temperature demanded less thermal exposure, the same pigment stayed stable enough for successful compounding — a result the authors read as evidence that pigment compatibility depends strongly on the thermal requirements of the matrix.

Rheological changes were modest. Melt flow rate fell slightly after pigment incorporation, pointing to a small rise in melt viscosity. Neat PLA measured about 50 g/10 min, and the natural-pigment masterbatches stayed close to that figure; PBS responded similarly, with only a minor reduction. The authors stress that this matters for compounders, since a color system forcing major changes to screw design, pressure settings or molding conditions would offer little practical value.

Tensile and impact behavior were also checked across the 2–6 wt% range. Neither polymer showed significant losses in overall mechanical performance. PLA started from a Young's modulus of about 1710 MPa and tensile strength of 65.6 MPa, PBS from about 392 MPa and 34.5 MPa, and the colored formulations remained close to those baselines. Impact strength stayed in a similar band, although individual pigments produced some variation.

Successful extrusion did not guarantee durable color. After 50 hours of xenon-lamp exposure, most formulations showed a color difference above ΔE* = 2, a shift the researchers describe as visually perceptible. The clearest exception was a PLA formulation containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability. The study identifies UV stability as the largest barrier to broader use, noting that packaging, consumer products, agricultural parts and outdoor applications may need additional stabilization, protective coatings or pigment modification before natural colors can compete with conventional systems over long service periods.

An environmental comparison favored the natural route under the study's assumptions. One kilogram of curcumin pigment corresponded to about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment, and the natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.

The authors conclude that natural pigment masterbatches still require development, particularly in lightfastness and thermal stability. Even so, the work shows that several natural colorants can be compounded into PLA and PBS on conventional processing equipment with only limited changes in melt viscosity and mechanical performance, and they argue that future effort should concentrate on color stability during processing and in later service exposure.