Renewable Energy

Emulsion buffer layer limits screen-printing degradation in copper-plated HJT solar cells

A Chinese research team linked the damage to worn screen-mesh knuckles and found that a 4.7% emulsion coverage ratio offered the best protection-uniformity trade-off.

Naledi MokoenaNovember 15, 20265 min read5 views

A fine screen-printing mesh is shown above a silicon solar cell wafer, with a thin emulsion layer separating the mesh knuckles from the wafer surface in a conceptual laboratory view.

Screen printing is a workhorse process in solar-cell metallization, but its mechanical and thermal demands can degrade device performance. The problem is especially acute for copper-plated silicon heterojunction (HJT) cells, which are being pursued as a route to lower metallization costs and reduce reliance on silver.

Researchers in China have investigated how screen printing damages copper-plated HJT cells and developed a modified screen design intended to limit the effect. Their focus was the photoresist-application step, not the conventional printing of silver paste.

Corresponding author Lang Zhou explained that photoresist printing differs fundamentally from silver-paste printing. In silver-paste printing, the screen openings occupy only 2–5% of the total area, while an emulsion layer covers the rest and prevents direct contact between the mesh and the wafer. Full-area photoresist coating typically uses a screen without emulsion coverage to spread resist uniformly across the wafer. As a result, the mesh comes into direct and extensive contact with the wafer during every printing cycle.

Earlier investigations cited by the team found conversion efficiency declining from 26.2% to 25.7% over 15,000 consecutive printing cycles in commercial solar cell production. The losses were mainly in open-circuit voltage and fill factor, while short-circuit current density and electrical resistance were largely unchanged. Minority-carrier-lifetime degradation rose from 0.61% with a new screen to 11.0% after 15,000 cycles.

Wear at the mesh knuckles

Using three-dimensional confocal microscopy, the researchers identified progressive wear of the screen mesh knuckles as the main cause. As the raised intersections wore down, their contact area with the wafer increased, placing greater mechanical stress on the passivation layers beneath. Scanning electron microscopy showed no visible surface scratches, but photoluminescence measurements indicated increased recombination losses, pointing to damage at the amorphous silicon/crystalline silicon interface.

To reduce direct contact, the team added an emulsion buffer layer to the screen. They evaluated six patterns with emulsion coverage ratios ranging from 2.9% to 16.6%. The results showed a trade-off: higher coverage protected the wafer but impaired photoresist coating uniformity and ink distribution. A 4.7% coverage ratio provided the best balance, limiting minority-carrier-lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity.

The researchers attributed the improvement to the emulsion layer preventing direct contact between the mesh and the wafer, thereby reducing cumulative mechanical damage to the sensitive passivation layers. Zhou said the findings show that a relatively simple screen-design change can substantially mitigate printing-induced degradation and offer a practical route to improving manufacturing reliability.

The study was published in Solar Energy as “Screen-printing photoresist induced efficiency degradation and mitigation in Cu-plated SHJ solar cells.” It appears amid growing interest in copper metallization. In April 2026, Nankai University researchers reported a silver-free HJT cell at 25.2% efficiency using plasma-induced interface engineering and copper electroplating, addressing adhesion, contact resistance and stability at the ITO interface. Separately, Forschungszentrum Jülich achieved 23.08% in a fully copper-metallized HJT cell, with a relatively small efficiency penalty versus silver metallization; cells using silver-copper paste on the front and silver contacts on the rear reached 23.95%. Those results underline copper's potential to cut silver use, while further process and electrical improvements remain necessary.